UNS S31803
Loading...
UNS S31803Chemical composition:
C | Si | Mn | P | S | Ni | Cr | Mo | N | |
Min | – | – | – | – | – | 4.5 | 2 | 2.5 | 0.08 |
Max | 0.03 | 1 | 2 | 0.03 | 0.02 | 6.5 | 23 | 3.5 | 0.2 |
UNS S31803Physical properties:
Specific heat(J/kg・K) | 460 | |
Resistivity(μΩ・cm) | 87.0 | |
Thermal conductivity(W/m・K) | 13.9 | |
Average coefficient of thermal expansion(10-6/℃) | 20–100℃ | 12.7 |
20–200℃ | 13.1 | |
20–300℃ | 13.5 | |
20–400℃ | 13.8 | |
Longitudinal modulus of elasticity(MPa) | 19.5 x 10^4 | |
Ferromagnetic | Yes | |
Melting point(℃) | 1420-1465 |
UNS S31803Mechanical properties:
0.2%Yield strength(N/mm2) | Tensile strength (N/mm2) |
Elongation (%) |
Hardness | |
≧ 450 | ≧ 655 | ≧ 25 | (Hv) | (HB) |
― | ― |
UNS S31803 Alloy properties:
Corrosion Resistance:
Steel | Critical point corrosion temperature(℃) | Critical crevice corrosion temperature (℃) |
S31803 | 50 | 25 |
SUS 316L | 10 | 0℃hereinafter |
Acid Corrosion Resistance:
Steel | Test conditions | |||||||||
Sulfuric acid 80°C | Hydrochloric acid 80°C | |||||||||
5% | 10% | 20% | 40% | 60% | 80% | 0.1% | 1% | 2% | 3% | |
S31803 | < 0.1 | 0.1 | 3.3 | 250.5 | 263.1 | 90.4 | < 0.1 | < 0.1 | 19 | 51.5 |
SUS316L | 1.1 | 2.9 | 20.1 | 291.3 | 72.0 | 11.1 | < 0.1 | 2.5 | 6.7 | 13.5 |