H08825
H08825Chemical composition:
Fe | Ni | Mo | Cu | Cr | C | Si | Mn | P | S | |
Min | Bal | 38 | 2.5 | 1.5 | 19.5 | ≤ | ||||
Max | 46 | 3.5 | 3.5 | 23.5 | 0.05 | 0.5 | 1 | 0.04 | 0.03 |
H08825Physical properties:
Density/g·cm³ | Melting point/℃ | Coefficient of linear expansion/(10⁶ ·℃)-1 | Thermal conductivity/W·(m·℃)-1 | Resistivity/μΩ ·m | Elastic modulus
E/MPa×10³ |
||
20~100℃ | 20~300℃ | 25℃ | 150℃ | 20℃ | |||
8.14 | 1350 | 12.6 | 14.7 | 12.3 | 14.4 | 1.12 | 195 |
H08825Mechanical properties:
The state of heat treatment of the material | Mechanical properties | |||
σb/MPa | σp0.2/MPa | &;/% | ψ/%% | |
Solution annealed tubes | 608~647 | 264~323 | 44~53 | —— |
H08825 Alloy properties:
The alloy has a pure austenite structure under solution conditions. However, at medium aging, carbides and intermetallic compounds can precipitate on austenite matrices and intergranular bodies, and these precipitated phases can impair the mechanical properties and corrosion resistance of the alloy.
H08825Uses of alloys:
Due to its wide range of corrosion resistance, this alloy is widely used in the chemical processing industry, hot seawater, and hydrometallurgical plants. It is mainly used to treat heat exchangers, pipes, valves, pumps, etc. in hot sulfuric acid, chloride-containing solution, sulfurous acid and other environments. It is also widely used in the field of wood pulp leachers and deep-source gas wells in the paper industry.
H08825Process performance:
Welding process: The usual welding method can be used, and nickel-based welding wire (00Cr22Ni61Mo9Nb) is recommended.
Heat Treatment: A suitable final heat treatment for this alloy is 940°C stable. The intermediate annealing temperature should be higher than 1050°C.
Relevant standards:
ASTM B 425,ASTM B 564,ASME SB 425,ASME SB 564,ASTM B 424, ASTM B 906, ASME SB 424, ASME SB 906, DIN 17750,, ISO 6208、ASTM B 163, ASTM B 423, ASTM B 704, ASTM B 705, ASTM B 751, ASTM B 775, ASTM B 829, ASME SB 163, ASME SB 423, ASME SB 704, ASME SB 705, ASME SB 751, ASME SB 775, ASME SB 829,ASTM B 366, ASME SB 366, DIN 17744