HuaNickel GH38Ais a Fe-Ni-Cr base superalloy that can be used at temperatures below 700°C. Elements such as aluminum and titanium are added to the alloy to form a precipitation-strengthening phase, and boron is added to purify and strengthen the grain boundaries. The alloy has high thermal strength when used below 700°C, as well as good cutting and welding properties.

GH38AChemical composition:

  Fe Cr Ni Ti C B Mn Si S P
Min Bal 10 18 2.3
Max 12.5 21 2.8 0.1 0.008 1 1 0.02 0.03

GH38APhysical properties:

Density 7.94g/cm³

Thermal conductivity

θ/℃ 100 200 300 400 500 600 700 800 900
α/[W/(m·℃)] 16.3 17.6 18.8 20.5 22.6 23.9 25.1 26.8 28.5

Coefficient of linear expansion

θ/℃ 20~100 20~200 20~300 20~400 20~500 20~600 20~700 20~800
α/(10-6℃-1) 15.4 16.0 16.6 17.0 17.5 17.9 18.2 18.9
θ/℃ 100~200 200~300 300~400 400~500 500~600 600~700 700~800 ——
α/(10-6℃-I) 16.6 17.7 18.4 19.4 19.6 20.5 23.4  

GH38AMechanical properties:

 

Standard number

 

Variety

 

Heat treatment

Room temperature performance 800℃ tensile properties Long-lasting performance at 800°C
σb/MPa σp0.2/MPa δ₅/% ψ/% Ak/J  

HBS

      σ/MPa τ/h
YB/T 5245 Hot rolled rods Standard heat treatment 784 441 15 15 23.5 302~241 294 20 20 Choose Measured

GH38AAlloy properties:

GH38Aalloy has lamellar Laves phase precipitation at grain boundaries after heat treatment.

GH38AUses of alloys:

HuaNickel GH38Aalloy is mainly used for hot end components such as turbine discs, combustion chamber housing parts, turbine housings, supports, shafts and blades below 700°C.

GH38AProcess performance:

Welding process:

Sampling/mm Pre-weld heat treatment θ/℃ Tensile properties Impact performance
σb/MPa σp0.2/MPa δ₅/% ψ/% Ak/J
 

 

 

 

D20 hot rolled rod

Non-vacuum induction furnace

+ Electroslag

 

Not brazed

20 936 668 24.8 26.0 729~81
8C0 349 35.5 73 78.4
900 98 —— 86.4~128 >226
 

1180℃×25min/AC

20 941 611~645 17.0 17.1 54.9
800 348 47.0 73~78 58.8
900 117 80~115.2 >137
 

1220℃×25min/AC

20 916 593 224~27.2 24.7 62.7
800 353 37.2~49.2 75.5 74.5
900 116 104~115.2 >216

Relevant standards:

GB/T14992 、YB/T 5245、HB/Z 140