GH3039
GH3039 Chemical composition:
Ni | Cr | Mo | AI | Ti | Nb | C | Fe | Mn | Si | P | S | Cu | |
Min | Bal | 19 | 1.8 | 0.35 | 0.35 | 0.9 | ≤ | ||||||
Max | 22 | 2.3 | 0.75 | 0.75 | 1.3 | 0.08 | 3 | 0.4 | 0.8 | 0.02 | 0.012 | 0.2 |
GH3039 Physical properties:
Density | 8.3g/cm³ | |
Resistivity | 20℃ | 1.18×10-⁶Ω·m |
Magnetic properties | not |
Coefficient of linear expansion
θ/℃ | α/(10-6℃-I) | θ/℃ | α/(10-6℃-1) | θ/℃ | α/(10-6℃-1) |
20~100 | 11.5 | 20~500 | 13.8 | 20~800 | 15.3 |
20~200 | 12.4 | 20~600 | 14.3 | 20~900 | 15.8 |
20~300 | 13.2 | 20~700 | 14.9 | 20~1000 | 16.4 |
20~400 | 13.5 | — |
Resilient performance
θ/℃ | 20 | 400 | 500 | 600 | 700 | 800 | 900 |
E/GPa | 196 | 162 | 160 | 147 | 134 | 98 | — |
Ep/GPa | 211 | 182 | 176 | 169 | 162 | 155 | 147 |
GH3039 Mechanical properties:
Standard number | variety | heat treatment | Stretch at room temperature | 800℃Stretch | ||||
σb/MPa | δ₅/% | ψ/% | σb/MPa | δ₅/% | ψ/% | |||
≥ | ||||||||
GJB 1952A | Cold-rolled plate | (1050~1090)℃/AC | 735 | 40 | — | 245 | 40 | —— |
GJB 2297A | Cold-drawn notched tubing | (1050~1080)℃/AC/WQ | 6850 | 40 | 245 | 40 | —— | |
GJB 3165A | Hot rolled forged rods | (1050~1080)℃/AC/OQ | 735 | 40 | — | 245 | 40 | 40 |
GJB 3317A | Hot rolled plate | (1050~1090)℃/AC | 735 | 40 | 45 | 245 | 40 | 50 |
GJB 3318A | Cold-rolled strip | (1050~1090)℃/AC | 7352 | 40 | — | — | — | |
GB/T 15062 | Cold drawing | (1050~1080)℃/WQ | 635 | 35 | — | — |
GH3039 Alloy properties:
HuaNickel GH3039 alloy supply state sheet has good hot working process plasticity and good stamping properties. It can be welded by argon arc welding, spot welding or seam welding, etc., and its welding performance is excellent, and the crack tendency of argon arc welding is small. The welding characteristics are close to that of GH3030 alloy. It can be welded in combination with alloys such as GH1140, GH3030 and GH3044. There is no precipitation of harmful phase in the alloy, the microstructure stability is good, and when working at high temperature for a long time, there is a tendency to oxidize along the grain boundary.
GH3039 Uses of alloys:
GH3039 alloy is used to make aero engine combustion chamber and afterburner parts.
GH3039 Process performance:
Welding process: The alloy can be welded by argon arc welding, spot welding or seam welding, which has excellent welding performance and small crack tendency of argon arc welding.
Plasticity of hot working process:HuaNickel GH3039 alloy has good plasticity of hot working process and good deformation performance. The heating temperature for forging is 1170°C, and the final forging is 900°C.
Heat treatment: After heat treatment, the oxide scale on the surface of the part can be removed by sand blowing or pickling.
Relevant standards:
GB/T15062、GJB 1952A 、GJB 2297A、GJB 2612 、GJB3165A、GJB3317A 、GJB3318A 、HB/Z140