HuaNickel GH2132 is a precipitation-hardening deformed superalloy composed of Fe-Ni-Cr and other elements, which has good high and low temperature strength and long-term stability, good corrosion resistance and thermal deformation performance, and has good processing plasticity and satisfactory welding performance.

GH2132 Chemical composition:

Fe Cr Ni Mo Ti B V Mn C AI  Si P S Cu
Min Bal 13.5 24 1 1.75 0.001 0.1 1
Max 16 27 1.5 2.35 0.01 0.5 2 0.08 0.4 1 0.03 0.02 0.25

GH2132 Physical properties:

Density 7.93g/cm³
Melting point 1364℃~1424℃

Resistivity

θ/℃ 100 200 300 400 500
α/[W/(m·℃)] 14.2 15.9 17.2 18.8 20.5
θ/℃ 600 700 800 900
α/[W/(m·℃)] 22.2 23.9 25.5 27.6

Thermal conductivity

θ/℃ 100 200 300 400 500
α/[W/(m·℃)] 14.2 15.9 17.2 18.8 20.5
θ/℃ 600 700 800 900
a/[W/(m·℃)] 22.2 23.9 25.5 27.6

GH2132 Mechanical properties:

Standard number Variety Heat treatment θ/℃ Tensile properties  

HBS

Combined long-lasting performance
σb/MPa σp0.2/MPa δ₅/% ψ/% σ/MPa τ/h τh/h
Q/3B4071 Hot rolled rods Standard heat treatment 20 ≥1035 ≥690 ≥18 ≥30 352~277
650 448 ≥25 >t

GH2132 Alloy properties:

After long-term aging at 650°C, G phase and cellular η phase were precipitated at the grain boundary, and the η phase showed Wechsler microstructure after 6000 h. When the alloy composition exceeds the specifications of the technical standard or some process is not in order, an excess of η, G and o phases can occur, and an abnormal cellular γ phase appears.

GH2132 Uses of alloys:

HuaNickel GH2132 alloy has been used in the manufacture of fasteners for aviation and aerospace engines.

GH2132 Process performance:

Welding process: The alloy has satisfactory welding performance, and can be welded by argon arc welding, spot welding, and seam welding. The alloy is welded in a solution state, and the aging treatment is carried out after welding. The strength coefficient of the TIG welding butt sonotre with aging treatment after welding is greater than 90%.

Relevant standards: