Chemical composition(mass fraction)(wt.%) of the GH4141
C(%) | Si(%) | Mn(%) | P(%) | S(%) | Cr(%) | Ni(%) | Mo(%) | Cu(%) | Co(%) | B(%) | Nb(%) | Al(%) | Ti(%) | Fe(%) |
---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
0.06 -0.12 | 0.50 | 0.50 | 0.015 | 0.015 | 18.00-20.00 | Bal | 9.00-10. 50 | 0.500 | 10.00-12.00 | 0.003 -0.010 | – | 1.40 -1.80 | 3.00-3.50 | ≤5.00 |
Mechanical Properties of steel grade GH4141
Yield Rp0.2 (MPa) |
Tensile Rm (MPa) |
Impact KV/Ku (J) |
Elongation A (%) |
Reduction in cross section on fracture Z (%) |
As-Heat-Treated Condition | Brinell hardness (HBW) |
---|---|---|---|---|---|---|
674 (≥) | 744 (≥) | 11 | 13 | 33 | Solution and Aging, Annealing, Ausaging, Q+T,etc | 314 |
Physical Properties of steel grade GH4141
Temperature (°C) |
Modulus of elasticity (GPa) |
Mean coefficient of thermal expansion 10-6/(°C) between 20(°C) and | Thermal conductivity (W/m·°C) |
Specific thermal capacity (J/kg·°C) |
Specific electrical resistivity (Ω mm²/m) |
Density (kg/dm³) |
Poisson’s coefficient, ν |
---|---|---|---|---|---|---|---|
31 | – | – | 0.14 | – | |||
557 | 823 | – | 24.3 | 434 | – | ||
112 | – | 33 | 42.2 | 114 | 311 |
Heat Treatment of steel grade GH4141
Heat treated : 1885°C – 1586°C
Technological Curves of steel grade GH4141